Durabilidade da união à dentina e liberação de cálcio promovidas por sistemas adesivos experimentais com adição de hidróxido de cálcio
Objective: This study investigated the calcium release (CaR) and long-term dentin bonding stability (DBS) of experimental self-etching adhesive systems containing calcium hydroxide. Methodology: Four adhesive systems were formulated including UDMA, HEMA, GDMA-P, TPO and diphenyl iodonium monomers as...
Na minha lista:
Autor principal: | |
---|---|
Outros Autores: | |
Formato: | doctoralThesis |
Idioma: | pt_BR |
Publicado em: |
Universidade Federal do Rio Grande do Norte
|
Assuntos: | |
Endereço do item: | https://repositorio.ufrn.br/handle/123456789/44681 |
Tags: |
Adicionar Tag
Sem tags, seja o primeiro a adicionar uma tag!
|
id |
ri-123456789-44681 |
---|---|
record_format |
dspace |
institution |
Repositório Institucional |
collection |
RI - UFRN |
language |
pt_BR |
topic |
Adesivos dentinários Hidróxido de cálcio Resistência de união |
spellingShingle |
Adesivos dentinários Hidróxido de cálcio Resistência de união Amorim, Débora Michelle Gonçalves de Durabilidade da união à dentina e liberação de cálcio promovidas por sistemas adesivos experimentais com adição de hidróxido de cálcio |
description |
Objective: This study investigated the calcium release (CaR) and long-term dentin
bonding stability (DBS) of experimental self-etching adhesive systems containing
calcium hydroxide. Methodology: Four adhesive systems were formulated including
UDMA, HEMA, GDMA-P, TPO and diphenyl iodonium monomers as photoinitiator
system, and ethanol/water as solvent with different mass fractions of calcium
hydroxide: 0% (control), 1%, 2% and 4%. DBS was measured by the microtensile bond
strength method in a microtensile testing machine. The middle third of dentin from 24
human third molars (n = 6) was used to bond the adhesive systems to a composite resin.
Stick-shaped samples (1 mm2) were obtained after 24 hours of immersion in distilled
water and tested immediately and after 12 months of storage in water. Data were
statistically evaluated using two-way ANOVA and Tukey's post-test (p < 0.05). CaR
was evaluated using a spectrophotometer. Disc specimens (6.0 mm in diameter x 0.3
mm thick) were produced (n = 4) and immersed in distilled water. Calcium
concentration was measured after 3 h to 168 h. Results: For DBS, adhesive systems
containing 0%, 1% and 4% calcium hydroxide had statistically similar means between
the immediate time points (24h) and 12 months. The adhesive system containing 2%
calcium hydroxide had a statistically higher bond strength in 12 months (p = 0.001). No
material released calcium up to 168 h after photoactivation. Conclusion: The inclusion
of 2% calcium hydroxide resulted in improved long-term bond strength to dentin.
However, the inclusion of calcium hydroxide in the experimental adhesive systems
tested was not able to release calcium. |
author2 |
Borges, Boniek Castillo Dutra |
author_facet |
Borges, Boniek Castillo Dutra Amorim, Débora Michelle Gonçalves de |
format |
doctoralThesis |
author |
Amorim, Débora Michelle Gonçalves de |
author_sort |
Amorim, Débora Michelle Gonçalves de |
title |
Durabilidade da união à dentina e liberação de cálcio promovidas por sistemas adesivos experimentais com adição de hidróxido de cálcio |
title_short |
Durabilidade da união à dentina e liberação de cálcio promovidas por sistemas adesivos experimentais com adição de hidróxido de cálcio |
title_full |
Durabilidade da união à dentina e liberação de cálcio promovidas por sistemas adesivos experimentais com adição de hidróxido de cálcio |
title_fullStr |
Durabilidade da união à dentina e liberação de cálcio promovidas por sistemas adesivos experimentais com adição de hidróxido de cálcio |
title_full_unstemmed |
Durabilidade da união à dentina e liberação de cálcio promovidas por sistemas adesivos experimentais com adição de hidróxido de cálcio |
title_sort |
durabilidade da união à dentina e liberação de cálcio promovidas por sistemas adesivos experimentais com adição de hidróxido de cálcio |
publisher |
Universidade Federal do Rio Grande do Norte |
publishDate |
2021 |
url |
https://repositorio.ufrn.br/handle/123456789/44681 |
work_keys_str_mv |
AT amorimdeboramichellegoncalvesde durabilidadedauniaoadentinaeliberacaodecalciopromovidasporsistemasadesivosexperimentaiscomadicaodehidroxidodecalcio |
_version_ |
1773959234734522368 |
spelling |
ri-123456789-446812022-05-02T15:16:42Z Durabilidade da união à dentina e liberação de cálcio promovidas por sistemas adesivos experimentais com adição de hidróxido de cálcio Amorim, Débora Michelle Gonçalves de Borges, Boniek Castillo Dutra http://lattes.cnpq.br/2300905249971948 http://lattes.cnpq.br/2710860035611527 Lima, Renally Bezerra Wanderley e http://lattes.cnpq.br/4630640936500286 Maia, Conceição Aparecida Dornelas Monteiro http://lattes.cnpq.br/9359973819672781 Araújo, Diana Ferreira Gadelha de http://lattes.cnpq.br/1341888013706536 Assunção, Isauremi Vieira de http://lattes.cnpq.br/1625804512028497 Adesivos dentinários Hidróxido de cálcio Resistência de união Objective: This study investigated the calcium release (CaR) and long-term dentin bonding stability (DBS) of experimental self-etching adhesive systems containing calcium hydroxide. Methodology: Four adhesive systems were formulated including UDMA, HEMA, GDMA-P, TPO and diphenyl iodonium monomers as photoinitiator system, and ethanol/water as solvent with different mass fractions of calcium hydroxide: 0% (control), 1%, 2% and 4%. DBS was measured by the microtensile bond strength method in a microtensile testing machine. The middle third of dentin from 24 human third molars (n = 6) was used to bond the adhesive systems to a composite resin. Stick-shaped samples (1 mm2) were obtained after 24 hours of immersion in distilled water and tested immediately and after 12 months of storage in water. Data were statistically evaluated using two-way ANOVA and Tukey's post-test (p < 0.05). CaR was evaluated using a spectrophotometer. Disc specimens (6.0 mm in diameter x 0.3 mm thick) were produced (n = 4) and immersed in distilled water. Calcium concentration was measured after 3 h to 168 h. Results: For DBS, adhesive systems containing 0%, 1% and 4% calcium hydroxide had statistically similar means between the immediate time points (24h) and 12 months. The adhesive system containing 2% calcium hydroxide had a statistically higher bond strength in 12 months (p = 0.001). No material released calcium up to 168 h after photoactivation. Conclusion: The inclusion of 2% calcium hydroxide resulted in improved long-term bond strength to dentin. However, the inclusion of calcium hydroxide in the experimental adhesive systems tested was not able to release calcium. Objetivo: Este estudo investigou a liberação de cálcio (CaR) e estabilidade de adesão à dentina em longo prazo (DBS) de sistemas adesivos autocondicionantes experimentais contendo hidróxido de cálcio. Metodologia: Quatro sistemas adesivos foram formulados incluindo monômeros UDMA, HEMA, GDMA-P, TPO e difenil iodônio como sistema fotoiniciador, e etanol / água como solvente com diferentes frações de massa de hidróxido de cálcio: 0% (controle), 1%, 2% e 4%. O DBS foi medido pelo método de microtração de resistência de união em máquina de ensaio de microtração. O terço médio da dentina de 24 terceiros molares humanos (n = 6) foi usado para unir os sistemas adesivos a uma resina composta. Amostras em forma de palitos (1 mm2 ) foram obtidas após 24 horas de imersão em água destilada e testadas imediatamente e após 12 meses de armazenamento em água. Os dados foram avaliados estatisticamente por meio de ANOVA de dois fatores e pós-teste de Tukey (p <0,05). O CaR foi avaliado por meio de espectrofotômetro. Os espécimes em discos (6,0 mm de diâmetro x 0,3 mm de espessura) foram produzidos (n = 4) e imersos em água destilada. A concentração de cálcio foi medida após 3 h até 168 h. Resultados: Para DBS, os sistemas adesivos contendo 0%, 1% e 4% de hidróxido de cálcio apresentaram médias estatisticamente semelhantes entre os pontos de tempo imediato (24h) e 12 meses. O sistema adesivo contendo 2% de hidróxido de cálcio apresentou resistência de união estatisticamente maior em 12 meses (p = 0,001). Nenhum material liberou cálcio até 168 h após a fotoativação. Conclusão: A inclusão de hidróxido de cálcio a 2% resultou na melhora da durabilidade de união à dentina a longo prazo. No entanto, a inclusão de hidróxido de cálcio aos sistemas adesivos experimentais testados não foi capaz de liberar cálcio. 2021-10-21T22:42:26Z 2021-10-21T22:42:26Z 2021-06-25 doctoralThesis AMORIM, Débora Michelle Gonçalves de. Durabilidade da união à dentina e liberação de cálcio promovidas por sistemas adesivos experimentais com adição de hidróxido de cálcio. 2021. 45f. Tese (Doutorado em Ciências Odontológicas) - Centro de Ciências da Saúde, Universidade Federal do Rio Grande do Norte, Natal, 2021. https://repositorio.ufrn.br/handle/123456789/44681 pt_BR Acesso Aberto application/pdf Universidade Federal do Rio Grande do Norte Brasil UFRN PROGRAMA DE PÓS-GRADUAÇÃO EM CIÊNCIAS ODONTOLÓGICAS |